Physical Properties | Metric | English | Comments |
---|---|---|---|
Specific Gr***ity | 1.11 g/cc | 1.11 g/cc | ASTM D 792 |
Linear Mold Shrinkage | 0.015 - 0.045 cm/cm @Thickness 3.20 mm |
0.015 - 0.045 in/in @Thickness 0.126 in |
ASTM D 955 |
Mechanical Properties | Metric | English | Comments |
Hardness, Shore A | 60 | 60 | 10 s delay; ASTM D 2240 |
Tensile Strength at Break | 8.27 MPa @Thickness 3.20 mm |
1200 psi @Thickness 0.126 in |
Break, Die C, 20 in/min (500 mm/min); ASTM D 412 |
Tensile Strength, Yield | 1.52 MPa @Strain 50.0 % |
220 psi @Strain 50.0 % |
Die C 0.125 in (3.2 mm); 20 in/min (500 mm/min); ASTM D 412 |
2.00 MPa @Strain 100 % |
290 psi @Strain 100 % |
Die C 0.125 in (3.2 mm); 20 in/min (500 mm/min); ASTM D 412 | |
3.93 MPa @Strain 300 % |
570 psi @Strain 300 % |
Die C 0.125 in (3.2 mm); 20 in/min (500 mm/min); ASTM D 412 | |
Elongation at Break | 500 % @Thickness 3.20 mm |
500 % @Thickness 0.126 in |
Die C, 20 in/min (500 mm/min); ASTM D 412 |
Tear Strength | 33.3 kN/m | 190 pli | Die C; ASTM D 624 |
Compression Set | 20 % @Temperature 23.0 °C, Time 79200 sec |
20 % @Temperature 73.4 °F, Time 22.0 hour |
Method B; Type 2; ASTM D 395 |
75 % @Temperature 70.0 °C, Time 79200 sec |
75 % @Temperature 158 °F, Time 22.0 hour |
Method B; Type 2; ASTM D 395 | |
Processing Properties | Metric | English | Comments |
Melt Temperature | 193 - 238 °C | 380 - 460 °F | |
Mold Temperature | 21.1 - 48.9 °C | 70.0 - 120 °F | |
Drying Temperature | 82.2 °C @Time 7200 - 14400 sec |
180 °F @Time 2.00 - 4.00 hour |
|
Moisture Content | <= 0.030 % | <= 0.030 % | |
Dew Point | <= -17.8 °C | <= 0.000 °F |